Steel | Energy in elastic area up to εy | Energy (Ut) in elastoplastic area between εy and εmáx | Energy in damaged area between εmáx and εy limits | Strain εy | Strain εmáx | Strain εu | Ductility |
Not corroded A284 Grade C steel | 0.3443 | 88.49 | 29.10 | 0.003 | 0.2148 | 0.295 | 53.70 |
Corroded A284 Grade C steel | 0.25 | 59.60 | 23.27 | 0.0025 | 0.185 | 0.263 | 46.25 |
Not corroded A36 steel | 0.46 | 37.71 | 22.98 | 0.0025 | 0.078 | 0.124 | 31.2 |
Corroded A36 steel | 0.35 | 20.97 | 15.04 | 0.0022 | 0.050 | 0.083 | 25.0 |