Type of Alloy | Yield Strength (MPA) | UTS (MPa) | Failure Strain (%) | Density (g/cc) | Reference |
UNS N10276: Ni superalloy (C276) | 204 2.4 mm thickness, 429˚C | 601 4.8 - 25.4 mm thickness, 538˚C | 56 1.6 - 4.7 mm thickness, 204˚C | 8.89 | [12] |
Cartridge Brass (70/30) | 76 - 448 (Depends on temper) | 303 - 896 (Depends on temper) | 66 | 8.53 | [13] |
SS304 steel | 215 | 505 | 70 | 8 | [14] |
Maraging steel ASTM A 538 | 2617 | 2693 | 6 | 8 | [15] |
Mild steel: S275 | 245 - 275 | 410 - 660 | 20 - 22 | 7.85 | [16] |
Ti-6Al-4V: Ti alloy | 880 - 920 | 900 - 950 | 5 - 18 | 4.5 | [17] |
AA 7075: Al alloy (T6) | 430 - 480 | 510 - 540 | 5 - 11 | 2.81 | [18] |
AA 2024: Al alloy | Min. 345 | Min. 427 | 5 | 2.78 | [19] |
AZ91: Mg alloy (Die cast alloy) | 160 | 230 | 3 | 1.81 | [20] [21] |
AZ31: Mg alloy | 200 | 260 | 15 | 1.77 | [22] |