Samples | Tensile Modulus (MPa) | Tensile Modulus Improvement (%) | Tensile Strength (MPa) | Tensile Strength Improvement (%) |
Neat PA6.6 | 2400 | - | 69.8 | - |
PA6.6 + 0.25 wt% CNF-TEGO | 2586 | 8 | 71.8 | 2.9 |
PA6.6 + 0.5 wt% CNF-TEGO | 2971 | 24 | 80.6 | 15.5 |
PA6.6 + 1 wt% CNF-TEGO | 2811 | 17 | 74.8 | 7.2 |
PA6.6 + 0.25 wt% CNF-GO | 3225 | 34 | 72.1 | 3.3 |
PA6.6 + 0.5 wt% CNF-GO | 2868 | 20 | 71.7 | 2.7 |
PA6.6 + 1 wt% CNF-GO | 3122 | 30 | 64.4 | −7.7 |