S/N | Temp of Recrystilization | Degree of Rolling (%) | Mechanical Properties | Z (%) | ||
Rm (Mpa) | Re (Mpa) | A (%) | ||||
1 | 300˚C | 15.5 | 413 | 357.8 | 26.8 | 67.1 |
2 | 29.8 | 463.8 | 439.5 | 18.9 | 62.7 | |
3 | 42.5 | 459 | 377 | 30 | 64.2 | |
4 | 56.2 | 447.1 | 311.2 | 37.9 | 64.9 | |
5 | 70.2 | 452.9 | 307 | 38.5 | 57.2 | |
6 | 400˚C | 15.5 | 363.2 | 148.9 | 57 | 75.4 |
7 | 29.8 | 370.8 | 156 | 54.2 | 70 | |
8 | 42.5 | 373.2 | 163.9 | 51.8 | 69.1 | |
9 | 56.2 | 392.7 | 193.4 | 55.4 | 74.3 | |
10 | 70.2 | 403.2 | 210.7 | 48.4 | 62.8 | |
11 | 500˚C | 15.5 | 347.9 | 125.3 | 63.7 | 73.2 |
12 | 29.8 | 351.4 | 132.9 | 59 | 75.2 | |
13 | 42.5 | 352.3 | 134.9 | 60.1 | 75.7 | |
14 | 56.2 | 348.4 | 140.6 | 57.4 | 70.9 | |
15 | 70.2 | 355.4 | 139.2 | 52.1 | 69.1 | |
16 | 650˚C | 15.5 | 305.2 | 72.8 | 81.8 | 82.3 |
17 | 29.8 | 310.1 | 76.2 | 70 | 78.2 | |
18 | 42.5 | 304 | 75.7 | 72.8 | 81.7 | |
19 | 56.2 | 312.5 | 78.7 | 76 | 76 | |
20 | 70.2 | 315.6 | 78.5 | 65.2 | 76.9 |